Research Article

Optical and Thermal Properties of Zn/Al-Layered Double Hydroxide Nanocomposite Intercalated with Sodium Dodecyl Sulfate

Table 1

The indexing and lattice parameters (, , and ) of the PXRD for the ZnrAl-LDH and LDH-SDS with different concentration of SDS.

Parameter (nm)Interlayer thicknessa

Zn2-Al-LDH0.302.640.880.4030.29
LDH-SDS 0.2 M0.307.672.552.0729.99
LDH-SDS 0.4 M0.307.742.582.1042.89
LDH-SDS 0.8 M0.307.782.592.1151.44
Zn3-Al-LDH0.302.650.880.4023.67
LDH-SDS 0.2 M0.307.812.602.1245.97
LDH-SDS 0.4 M0.307.662.552.0728.07
LDH-SDS 0.8 M0.307.762.582.1034.38
Zn4-Al-LDH0.302.660.880.4028.85
LDH-SDS 0.2 M0.307.692.562.0823.42
LDH-SDS 0.4 M0.307.842.652.1231.57
LDHS-DS 0.8 M0.307.732.572.0933.09

Interlayer thickness = (—brucite-like sheet thickness).
(average crystallite size in direction) = value calculated from the values of (003), (006), and (009) diffraction peaks using the Scherrer equation.