Optimized PV performance for BHJ solar cells with Ag NPs under AM 1.5 G-simulated solar illumination (100 mW/cm2).

Amount of Ag NPs in 1 mL PEDOT:PSS [µL] [mA/cm2] [V]FF [—]PCEav. [%] [μW]PCEmax after 8 months [%] (lost, %)

ITO/PEDOT:PSS:Ag NPs/P3HT:PCBM/Al
08.58 (±0.20)0.598 (±0.001)0.57 (±0.02)2.77 (±0.11)1371.93 (30%)
607.36 (±0.13)0.604 (±0.002)0.49 (±0.05)2.16 (±0.24)1091.56 (28%)
907.36 (±0.09)0.607 (±0.002)0.46 (±0.03)2.05 (±0.17)1001.79 (13%)
1207.26 (±0.24)0.604 (±0.002)0.46 (±0.08)2.00 (±0.42)1101.07 (47%)
1506.81 (±0.03)0.557 (±0.003)0.47 (±0.01)1.80 (±0.02)821.50 (17%)

: open circuit voltage, : short circuit current density, FF: fill factor, PCE: power conversion efficiency, and : the maximum power of the pixel with PCEmax.