Study on the Microstructure of Vanadium-Modified Tungsten High-Speed Steel-Coded SAE-AISI T1 Steel
Table 9
Secondary hardening temperature and hardness values of investigating steels.
| Designation | Austenitization temperature | 1100°C | 1150°C | 1200°C | 1250°C | | | T | H | T | H | T | H |
| Standard T1 high-speed tool steel | 1V-18W | 525 | 61 | 525 | 62 | 550 | 64 | 550 | 65 |
| Vanadium-modified T1 high-speed tool steel | 2V-13W | 525 | 60 | 525 | 62 | 525 | 63 | 525 | 64 | 3V-8W | 525 | 60 | 525 | 61 | 550 | 62 | 525 | 63 | 4V-3W | 525 | 59 | 525 | 61 | 525 | 62 | 550 | 63 |
| Vanadium with extra carbon-modified T1 high-speed tool steel | 2V-13W–HC | 525 | 60 | 525 | 64 | 525 | 65 | 550 | 66 | 3V-8W-HC | 525 | 63 | 525 | 64 | 550 | 65 | 550 | 67 | 4V-3W-HC | 525 | 64 | 550 | 65 | 525 | 66 | 550 | 67 |
|
|
T: tempering temperature; H: hardness value. |